KC feed preparation (5 replies and 3 comments)
If you can somehow manage to use 2-3 mm screen apertures you will reduce the amount of coarse steel out-competing fine gold in the concentrator and greatly reduce your bowl wear rates.
Assuming you are only treating a portion of the CUF by gravity you will need less mag-sep capacity by treating a bleed stream (like the scalping screen feed). Drawing down your recirculating tramp steel load works just like gravity recovery of gold, by treating any portion of the circulating load you will be pulling out steal that will eventually report to your concentrator. I have even seem mag-sep units treating concentrator tailings to keep the steel from getting back to the mill.
Will reducing the KC feed size eliminate or rather it will allow finer sized metal into the KC, which again will be problematic during intensive cyanidation. Remember there would be no point where the steel is removed from the grinding circuit
This will not eliminate steel to the gravity concentrator but it is the easiest way to minimize the amount of steel getting into your concentrate, will likely lead to an increase in gravity recovery and give you longer bowl life; this is assuming your scalping screen is large enough to handle 2 mm apertures.
If the steel is causing problems in the intensive leach why not put your mag-sep on the gravity concentrate stream before entering the leach reactor?
I have heard of excessive amounts of steel causing issues in ILRs before but haven't experienced it in person. Can you describe your ILR circuit and what % steel you are talking about?
As Gene and sagmill70 implied, tramp iron from broken balls and other sources will always be coming out of your mill. Removing it has been a major milling issue almost from the beginning of SAG milling (and other milling also). This is one of the reasons almost all SAG mills (and AG mills) have their discharge screened, with the oversize being conveyed to a crushing circuit or back to the feed with a tramp iron magnet on the conveyor. I have heard of an attempt to have the discharge in a sluice with a magnet over the sluice, but never heard of how it worked out.
I am having problems with the amount of tramp metal (from grinding media) that ends up in my knelson concentrator and subsequently affecting recovery. The KC is treating SAG mill primary cyclone underflow, KC feed size 4.5mm, KC model XD 30. Which is the best place to remove tramp metal, from the grinding circuit. The mill discharge or on the KC vibro feed screen?